09.12.2025

Heat transfer vinyl cracks on knitwear: what to change

Heat transfer vinyl cracks on knitwear: what to change

If heat transfer vinyl cracks inside the design when the T-shirt is pulled on while the edges hold, the film cannot stretch with the knit: it is too thick, overheated in the press or placed where the fabric stretches most. Pressing again will not close the cracks. For the next garment, use a thin polyurethane film, press it exactly as the product card says and test a sample on a person.

First, check what has come apart

Inspect the fully cooled design with the fabric relaxed, then stretch the fabric gently as it would stretch on the body. Do not pick at the edges or pull it to its limit.

  • A line opens within the film, but both halves stay against the fabric — the film itself has split.
  • An edge has lifted, leaving a gap underneath — the film has not bonded properly. Cover the design with a teflon sheet and press for 5–10 s at the film settings. If the edge lifts again, the squares test in the article “Heat transfer vinyl lifts with the carrier” will show the cause.

Both can happen at once. Pressing an edge down will not close a crack.

Cracks only appeared after a few washes? Check the care first: the article “Why heat transfer vinyl wrinkles after washing” has a care note for buyers.

The adhesive holds, but the film cannot stretch far enough

Knit fabric lengthens as its loops open out. The bonded design has to move with it. When the fabric lengthens more than the film can, the film tears while the adhesive keeps the pieces in place.

FilmAdhesiveKnit fabric

Intact design

Without excessive strain

Split film

← Fabric stretches →

The pieces are bonded, with a split between them

Cross-section of the design on a T-shirt.

Film and settings

For cotton or polyester/cotton knit fabric, use a thin MyPrint polyurethane film, for example the white film, 0.09 mm thick. The settings from its product card for a flat heat press:

MyPrint polyurethane film

Temperature150–160 °C
Time10–15 s
PressureMedium
Carrier removalCold peel

The same settings apply to every colour of this film. Do not press hotter than 160 °C or longer than 15 s: overheated film turns brittle and cracks even on an ordinary cotton T-shirt. If you pressed hotter or longer, repeat the test at the card settings first. For knitwear, use polyurethane film: it is thinner and softer than PVC (0.09 vs 0.11 mm), while glitter film (0.25 mm) and mesh glitter (0.4–0.5 mm) are several times thicker. On close-fitting elastane knits even polyurethane can crack; the test will show it.

Test a sample on a person

  1. Choose the placement. Put the blank on a person of the right size and draw a 10 cm chalk line wherever the design could go. Ask them to raise their arms and measure the lines again. Place the design where the line stretched least.
  2. Cut the sample at full size. Cut the widest solid part of the design with a cutting plotter: a small fragment will not show cracks.
  3. Apply it to a T-shirt from the same batch. Lay it on the platen without tension: fabric stretched “to spare” shrinks back after pressing and gathers the film into waves. Press at the card settings and peel the carrier once cool. Do not try on or fold the finished garment until the design has cooled.
  4. The next day, put the T-shirt on and take it off several times. Then ask the wearer to raise their arms and stretch. Inspect the design on the person: there should be no cracks or lifted edges.

A large solid fill in an area that stretches cracks first. If the customer agrees, make it narrower or split it into parts with gaps: the fabric between them then takes most of the stretch, not the film.

What to do with the result

The design is intact and the edges lie flat. Wash the sample inside out at 40 °C, dry it and put it on again. If the design is still intact, start the batch.

A crack appeared. Move the design to where the line stretched less, use a looser blank or make the solid fill narrower, then repeat the test.

Pressing again will not mend torn film: the crack reopens at the first stretch, and the extra heat makes the film even more brittle. Keep the spoiled T-shirt for tests and make the customer a new one with a film, settings and placement that passed the test.